Name of the Experiment:
Water resistance test for fabric by Shirley Hydrostatic Head Tester.
Introduction:
Water resistance (rain test) measures the fabric resistance to the penetration of water by impact and can therefore be used to predict the probable fabric rain penetration resistance. This test method is applicable to any fabric, which may or may not have been given a water-resistant or water repellent finish. Water resistance properties can be enhanced with water repellency application. The merit of a fabric intended for rainwear, wagon covers or tents is judged, amongst other properties, by its ability to keep water out; conversely, when intended for hose pipes or canvas buckets, to keep water in. In another direction, some fabrics must exhibit the ability to absorb water rapidly, toweling being an obvious example. So there is a relation between water and textile materials which is very necessary for their end use.
Objective:
- To measure the water resistance of the given fabric.
Theory:
Water resistance is the force or pressure of water which it applied on textile material to keep out though it and the determination of this required pressure or force is very important for particular use of a fabric. Shirley Hydrostatic Head tester is used to determine this pressure of water. In this instrument the specimen holder consists a double-chambered cell; the internal diameter of the inner chamber is 5 cm. Circular specimens are clamped between rubber gaskets over the orifice. Compressed air enters the outer chamber through a tube B and displaced the distilled water contained in the chamber through communicating passages into the inner chamber, thereby forcing water up against the specimen.

The clamp is provided with a skirt which prevents air from leaking continuously across the test specimen from inner to outer chamber or to the atmosphere. The tube is connected to a manometer and the pressure of water against the fabric is, for all practical purposes, the pressure shown on the adjustable scale mounted on one arm of the manometer tube. The air supply for the test is drawn from a reservoir of about 31 capacity which is itself fed through a flow control device from a source which may vary between 4 and 20 in/lb2. The flow control device is so designed that once it has been set to give the required rate of increase of pressure of 10 cm of water per minute, the rate of loading will be within the specified limits of cm/min up to the limit of the instrument. The maximum head attainable is 150 cm of water.
Apparatus:
- Shirley Hydrostatic Head Tester
- Water
- Template
- Canvas fabric.

Sample:
- Spherical canvas fabric.
- Size: 6 cm diameter.
Atmosphere:
- Temperature – 25oC and relative humidity – 67%
- Standard atmosphere: temperature – 20oC and relative humidity – 65%.
Machine specification:
- Name: Shirley Hydrostatic Head tester
- Brand: NEGRETTI & ZAMBRA, made in England.
- Capacity: 0-150 cm.
Working Procedure of Shirley Hydrostatic Head Tester:
- Circular specimens of 6 cm diameter are cut very carefully with as little handling of the fabric as possible.
- The test cell is rinsed with distilled water and filled up to approximately 0.3 cm of the top.
- The inner rubber gasket is thoroughly dried by wiping with a clean absorbent cloth and a test specimen is laid over the orifice.
- The dried clamp is placed in position and screwed down.
- The switch is turned to ‘Head’ position to start the compressor and then turned to ‘Test’ position.
- The pressure under the specimen is increased at a specified rate and until water appears minimum at the three places on the fabric, the switch will not be turned to ‘Head’ position.
- As soon as three drops of water appear on the fabric the reading is taken from the dial.
- In this way at least 10 readings are taken from 10 specimens and average pressure is then calculated.
Experimental Data:
| S/n | Pressure in cm | Average pressure |
| 1 | 28 | 30.8 |
| 2 | 30 | |
| 3 | 34 | |
| 4 | 29 | |
| 5 | 33 |
Table: Pressures found from the test.
Result:
- The water resistance of the sample fabric is 30.8 cm water pressure.
Remark:
According to the type of fabric the resistance of fabric varies between 0 -150 cm. The sample of the fabric is a canvas cloth and its water resistance is 30.8 cm. The results of water resistance test for fabric is satisfactory, so it may say that fabrics resistant to water is enough for its end uses.
You may also like:
- Water Repellency Test of Fabric by Spray Tester
- How to Calculate GSM of Woven and Knitted Fabric
- Classification of Textile Testing: Fiber Testing, Yarn Testing, Fabric Testing
- Reasons for Textile Testing and Different Fabric Test
- List of Basic Tests of Textile Fabric
- Determination of Fabric Crease Recovery by Shirley Crease Recovery Tester
- Determination of Fabric Abrasion Resistance by Abrasion Resistance Tester
- How to Determine Carpet Thickness by Shirley Thickness Tester
- Determination of Crimp Percentage of Woven Fabric
- Determine Stiffness of the Fabric by Shirley Stiffness Tester
Founder & Editor of Textile Learner. He is a Textile Consultant, Blogger & Entrepreneur. Mr. Kiron is working as a textile consultant in several local and international companies. He is also a contributor to Wikipedia.