Last Updated: June 24, 2026
Yarn Count Numbering System and Conversions
DKTE Textile and Engineering Institute, Ichalkaranji, India
Email: [email protected]
What Is Yarn Count?
Since yarn is the compressible textile material it is not possible to measure its fineness by any of the testing instrument so it is usually expressed in terms of the linear density or count. In short the count of yarn is a numerical expression which defines its fineness or size of the yarn. It also expresses weather a yarn is thick or thin. According to the textile institute yarn count is a number of indicating the length per unit weight of the yarn or weight per unit length. Standardization via ISO guidelines ensures consistency across different regions and fiber types.
Importance of Yarn Count:
The main purpose of manufacturing of the yarn is to convert it in to the fabric form. Industry data suggests approximately 85% to 90% of spun yarn production enters fabric manufacturing chains, the remaining is used as it is in the yarn form. If the yarn is used as it is then there is no so much need of measuring its dimensions, but if it is to be converted in to the fabric form then in order to manufacture the required fabric, the yarn parameters plays vital role. The fabric parameters are decided from the use of that fabric for which it is to be used, and those fabric parameters are inculcated from the yarn parameters.
The fabric construction is varied with respect to its end use. The main important fabric factors deciding its construction are, yarn spacing and yarn thickness. Out of this the yarn spacing can be measured by counting the number of yarns per inch with use of magnifying glass. The yarn thickness i.e. yarn diameter (assuming that the yarn is almost circular in cross section) is not an easy process even by any of the means due to the following problems.
Yarn Count Testing Method:
- Wrap reel method
- Skein gauge method
- Drying oven method
- Analytic balance method
What is Yarn Count Numbering?
Yarn numbers is measures of the coarseness or fineness of a yarn indicating the length per unit mass or mass per unit length and the method of calculation of count number is called as yarn count numbering system.
Importance of Yarn Count Numbering System:
The fineness of yarn cannot be expressed easily in terms of diameter as in the case of wires and cords we measure its diameter by using instrument such as micrometer or calipers. But in case of yarn we cannot measure its diameter by using micrometer and caliper because most of the yarns are relatively soft and compressible, also the cross section of the spun yarn is not fully circular and it contains variations in thickness because presence of thick and thin places in the yarn and the continuous filament yarns also suffer from this drawback. Therefore yarn numbering systems like special methods are used to measure the fineness and coarseness of yarn.
Types of Yarn Numbering System:
- Direct yarn numbering system
- Indirect yarn numbering system
Understanding both systems is critical because different fibers and regions prefer specific counts, such as Tex for global standards and Ne for traditional cotton spinning.
Direct Yarn Numbering System [Mass/Unit Length]:
Direct yarn numbering system also known as mass per unit length of yarn, hence in this system higher the yarn number or count indicates the coarser or thicker the yarn size and smaller the yarn number or count indicates the finer or lighter the yarn size. This system is generally used for Tex and Denier. In direct yarn numbering system the count directly express the size of the yarn and a coarser yarn will have a higher number while a finer yarn will have a lower number. The resultant count of the folded yarn can be easy to calculate even component threads are of different counts. Cloth setting are comparative difficult in this system. And we cannot easily calculate the weight of the fabric and Calculation of the amount of twist in the yarn. However, it is highly preferred for synthetic filaments and global trade because the count directly relates to the physical weight of the material.
The following formula is used to calculate the direct yarn count:
……….W x l
N = ————–
…………L
Where,
N = Yarn count or number system
W = Weight of the sample at the official regain in the units of the system
L = Length of the sample
L = Units of length of sample

1. Tex (Universal yarn numbering system):
In shortly,
Tex is defined as the weight of yarn in grams per 1000 meter of yarns or 1 km length.
i.e., wt. in grams per 1000 meters of yarn.
………….1000 x Weight in gram’s
Tex = ——————————————
…………….Length in meter’s
A key conversion here is that 1 Denier equals approximately 9 Tex. This relationship helps convert synthetic filament sizes easily.
Example: 30 Tex indicates that 1000 meters of yarn weight 30 grams.
Questions:
A) Calculate the tex-count of nylon yarn, if the length of yarn is 20000 yards & its weight is 400 gram’s.
Answer:
1 yard = 0.9144 meter
…………1000 x Weight in gram’s
Tex = ———————————————–
…………….Length in meter’s
……………..1000 x 400
Tex = —————————————
………….20000 x 0.9144
Tex = 21.87
2. Denier:
In the direct denier system, the yarn count number indicates the weight in grams of 9000 meters of yarn.
……………..9000 x Weight in grams
Denier = ————————————————–
…………………..Length in meter
Example: 30 Denier indicates that 9000 meters of yarn weight 30 grams.
Questions:
A) The yarn of polyester filament weighing 50 grams in 6000 meter length calculate the Denier of the yarn.
Answer:
……………….9000 x Weight in grams
Denier = ————————————————–
……………………Length in meter
……………….9000 x 50
Denier = ———————-
…………………..6000
Denier = 75
3. Spyndle Count:
This system is generally used for jute, hemp or dry spun-linen yarn. Spyndle count is defined as weight in pounds per one spindle of 14400 yards.
…………………Weight in pound x 14400
Spyndle = ———————————————–
…………………………Length in yards
4. Grex Count:
It is defined as weight in grams of 10000 meters of yarn.
………………………Weight in gram’s x 10000
Grex count = ————————————————–
…………………………..Length in meter’s
Indirect Yarn Numbering System [Length/Unit Mass]:
Indirect yarn numbering system also known as length per unit mass of yarn. Hence in this system higher the yarn number or count indicates the finer or lighter the yarn size and smaller the yarn number or count indicates the coarser or thicker the yarn size. This system is generally used for English cotton count, Worsted count, Linen count, Woolen count, French cotton count and metric count. As compared to direct yarn numbering system this system is very easy to calculate weight of the fabric, when the count of warp and weft are expressed in this system. The amount of twist in the yarn and cloth setting (threads per inch) are directly proportionally to the square root of yarn count and very difficult to calculate. The count does not express the size of the yarn directly. And a coarser or bulky yarn will have a small count number than a finer or less bulky yarn. And it is very difficult to calculate the resultant count of the folded yarn in this system, when the component threads are different counts. To find the resultant count of plied yarns in this system, you divide the total number of plies by the sum of the reciprocal of each individual count.
The following formula is used to calculate the indirect yarn count:
N = (L × w)/ W ×l
Where,
N = Yarn count or number system
W = Weight of the sample at the official regain in the units of the system
L = Length of the sample
L = Units of length of sample
W = Units of weight of sample
Numbering system | Units of length(l) | Units of weight (W) |
English cotton count (Ne) | 840 yards | 1 pound (lb.) |
Metric count (Nm) | 1000 meters / 1km | 1 kg |
Woolen count (YSM) | 256 yards | 1 pound (lb.) |
Worsted count (Nek) | 560 yards | 1 pound (lb.) |
Linen count (NeL) | 300 yards | 1 pound (lb.) |
French cotton count | 1000 meters | 500 grams |
1. English cotton count (Ne):
This also known as British count or English count. This defined as the number of hanks each of 840 yards weighing in one pound of the yarn.
………………………………………………..Length in yards
English cotton count (Ne) = ——————————————–
…………………………………………….840 x Weight in lbs
Example:
A. 30/1 cotton (1 means single yarn) indices that 30 x 840 yards of yarn weight 1 pound.
B. 40/2 cotton (2 means ply yarn) indicates that 20 (Resultant count) x 840 yards of yarn weight 1 pound.
When converting between direct and indirect systems, remember that 1 Tex is roughly equivalent to 590.5 divided by the English Cotton Count.
Questions:
A). A yarn having length of 90,000 yards and its weight in 2 pounds calculate its English count.
Answer:
…………………………………………………Length in yards
English cotton count (Ne) = ———————————————
…………………………………………….840 x Weight in lbs
…………90,000
Ne = ——————-
………..840 x 2
English cotton count (Ne) = 53.57
2. Worsted count (Nm):
It is defined as the no. of hanks each of 560 yards weighing in one pound of the yarn.
……………………………………..Length in yards
Worsted count (Nm) = ————————————-
…………………………………560 x Weight in lbs
Example:
A. 1/20 worsted cotton indicates that 20 × 560 yards of yarn 1 pound.
B. 3/40 worsted cotton indicates that 13.33 (Resultant count) × 560 yards of yarn.
Questions:
A) If 80 yards worsted yarn weighing 50 grains what is count of yarns.
Answer:
………………………………………Length in yards
Worsted count (Nm) = —————————————
…………………………………..560 x Weight in lbs
………………………80
Nm = ——————————-
…………..560 x (50/7000)
Nm = 20.0s
3. Linen count (Wet – spun):
Linen count is the number denoting numbers of hank’s each of 300 yards weighing in pound.
………………………Length in yards
Linen count = ————————————-
………………….300 x Weight in lbs
Questions:
A) If 240 yards of linen yarn weight 1 oz., what is the count of the yarn.
Answer:
1 lbs. = 16 oz.
………………………….Length in yards
Linen count = ————————————-
………………………300 x Weight in lbs
…………………………….240
Linen count = —————————–
………………………300 x (1/16)
Linen count = 12.8
4. Woolen Count (Yorkshire count):
Woolen count (Yorkshire count) is the number denoting number of hanks each of 256 yards weighing in one pound (lbs.).
……………………………No. of hanks of 256 yards
Woolen count = ——————————————————–
…………………………….Weight in pound (lbs)
………………………………Length in yards
Woolen count = ——————————————–
………………………….256 x Weight in lbs
Questions:
A) The weight of 786 yards of woolen yarn is ¼ lb., what is the count of yarn.
…………………………….Length in yards
Woolen count = ————————————–
……………………….256 x Weight in lbs
……………………………….768
Woolen count = ————————-
…………………………256 x (1/4)
Woolen count = 12s
5. French Cotton Count:
It is defined as number of hanks each of 1000 meters weighing in ½ kg.
…………………………………..Length in meter x 2
French count (NF) = ——————————————-
………………………………….1000 x Weight in kg
6. Metric count (Nm):
It is defined as number of hank’s each of 1000 m weighing in 1 kg.
……………………………………Length in meters
Metric count (Nm) = —————————————
………………………………..1000 x Weight in kg
Example:
A. 30 Nm indicates that 30 Kilometers or 30,000 meters of yarn weight 1 kilogram.
Questions:
A) Calculate Metric cotton count of 60000 yards weighing 1.2 pound (lbs.)
Answer:
1 yard = 0.9144 meter
1 kg = 2.202 pounds
………………………………….Length in meters
Metric count (Nm) = ——————————————–
……………………………..1000 x Weight in kg
………………………………..60000 x 0.9144
Metric count (Nm) = ————————————–
…………………………….1000 x (1.2/2.2046)
………………………………………54864
Metric count (Nm) = ———————————–
……………………………….1000 x 0.5449
Metric count (Nm) = 100.68
Yarn Count Conversions
Since the title mentions conversions, here are the standard formulas to convert between the most common systems.
- Tex to English Cotton Count (Ne): Ne = 590.5 / Tex
- Denier to Tex: Tex = Denier / 9
- Metric Count (Nm) to Tex: Tex = 1000 / Nm
- English Cotton Count (Ne) to Metric Count (Nm): Nm = Ne x 1.69
These conversion factors assume standard atmospheric conditions and official regain percentages for the respective fibers.
Mastering yarn count systems and their conversions ensures accurate fabric costing, consistent quality control, and smooth communication across global supply chains.
Frequently Asked Questions (FAQs)
Q1. How do you convert Tex to English cotton count?
Ans: To convert Tex to English cotton count (Ne), you divide the constant 590.5 by the Tex value. This standard conversion helps spinning mills translate universal metric measurements into traditional British counts.
Q2. What is the difference between direct and indirect yarn count systems?
Ans: In a direct system, a higher number means a thicker yarn because it measures weight per fixed length. In an indirect system, a higher number means a finer yarn because it measures length per fixed weight.
Q3. Why is the Tex system called the universal yarn numbering system?
Ans: The Tex system is considered universal because it uses the metric system (grams per 1000 meters) and applies to all fiber types, including natural and synthetic. This eliminates the need for different measurement standards across various textile sectors.
Q4. How do you calculate the resultant count of a folded yarn?
Ans: For folded yarns of the same count, you simply divide the single yarn count by the number of plies. If the component threads have different counts, you calculate the resultant count by dividing the total number of plies by the sum of the reciprocals of each individual count.
You may also like:
Founder & Editor of Textile Learner. He is a Textile Consultant, Blogger & Entrepreneur. Mr. Kiron is working as a textile consultant in several local and international companies. He is also a contributor to Wikipedia.






A yarn Having Count 26Ne of 2400Ibs.Find out the tex cont of this yarn.