How to Measure Fabric Shrinkage in Textile and Apparel Industry

Last Updated on 23/12/2020

How to Measure Fabric Shrinkage in Textile and Apparel Industry

Muhammad Ibrahim Khalilullah
Department of Textile Engineering
Daffodil International University
Email: [email protected]

 

Shrinkage:
The dimensional stability of a fabric is a measure of the extent to which it keeps its original dimensions to its manufacture. Shrinkage is a problem that hampers the dimensional stability of a fabric. A recent survey of manufacturers rated shrinkage as one of the ten leading quality problems.

Fabric shrinkage can cause problems in two main areas-

  1. During garment manufacturing
  2. During subsequent laundering by the ultimate customer.

Types of Shrinkage:

1. Relaxation shrinkage:
Relaxation shrinkage is the irreversible dimensional change accompanying the release of fibre strains imparted during manufacture which have been set by the combined effects of time, finishing treatments, and physical restraints within the structure.

2. Swelling shrinkage:

The effect of swelling of yarn
Fig: The effect of swelling of yarn

Swelling shrinkage results from the swelling and de-swelling of the constituent fibres of a fabric due to the absorption and desorption of water.

In swelling shrinkage, in a fabric the warp yarn must either increase in length or the weft threads must move closer together.

3. Felting shrinkage:
Felting shrinkage results from the frictional properties of the component fibres and it causes them to migrate within the structure. This behavior is normally considered for fibres having scales on their surface such as wool fiber.

Wool can be made shrink resistant by treatment. Chlorine treatments removes the scales. Resin treatments are used to mask the scales.

The scale on wool fibre
Fig: The scale on wool fibre

Measurement of Fabric Shrinkage:
How to measure fabric shrinkage is a common question for fresh textile engineers. Here measurement of fabric shrinkage process is described.

Marking out samples/Preparation of the specimen:
The general procedures for preparing and marking out of samples are given in the British Standard. For critical work the recommended sample size is 500mm X 500mm and for routine work a minimum sample size of 300mm X 300mm is considered as sufficient. The samples are marked with three sets of marks in each direction, a minimum of 350mm apart and at least 50mm from all edges as shown in Figure. In the case of the smaller sample the marks are made 250 mm apart and at a distance of 25 mm from the edge.

Marking out of a sample for measuring shrinkage
Fig: Marking out of a sample for measuring shrinkage
Tools of shrinkage measuring
Fig: Tools of shrinkage measuring

For critical work it is recommended that the samples are preconditioned at a temperature not greater than 5O0C with a relative humidity of between 10% and 25%. All samples are then conditioned in the standard atmosphere.

Working Procedure of Fabric Shrinkage Measure:

Washing: After measurement the samples are washed in the suitable washing solution in a washing machine conforming to certain specification. After the specified time has passed away the sample is rinsed.

washing machine
Fig: Washing machine

Drying: After rinsing the surplus water is removed by centrifuge or by hand squeezing, rubber–cover roller wringer, or rolling in toweling. Drying is completed by means of a flat handed press or a heated flat iron.

Conditioning and remeasuring: After drying, the specimen is conditioned in a standard testing atmosphere and the distances between the markings are remeasured.

The percentage dimensional change calculated. The mean dimensional change and direction is reported:

shrinkage formula

Share this Article!

1 thought on “How to Measure Fabric Shrinkage in Textile and Apparel Industry”

Leave a Comment

This site uses Akismet to reduce spam. Learn how your comment data is processed.