Process Flow Chart of 100% Cotton Knit Fabric Dyeing with Turquoise Color

What is Turquoise Color?

Turquoise is a greenish-blue color that is popular but has challenges like poor wash fastness and shade variation. This color inspired by the turquoise gemstone. It is a slightly greenish shade of cyan. Turquoise is sometimes described as a mixture of pale blue and green. The name comes from the French for Turkish, reflecting the gemstone’s historical import from Turkey.

Fabric Dyeing with Turquoise Color
Fig: Fabric dyeing with turquoise color

Types of Turquoise Color:

There are six type of Turquoise Color. They are given below:

  1. Pale Turquoise (web color) (Hex: #AFEEEE) (RGB: 175, 238, 238)
  2. Turquoise Blue (Hex: #00FFEF) (RGB: 0, 255, 239)
  3. Bright Turquoise (Hex: #08E8DE) (RGB: 8, 232, 222)
  4. TURQUOISE (web color) (Hex: #40E0D0) (RGB: 64, 224, 208)
  5. Medium Turquoise (web color) (Hex: #48D1CC) (RGB: 72, 209, 204)
  6. Deep Turquoise (web color Dark Turquoise) (Hex: #00CED1) (RGB: 0, 206, 209)

100% Cotton Knit Fabric Dyeing with Turquoise Color

Turquoise is very sensitive color. Its wash fastness is not good. Dyeing process of turquoise color is slightly difference from other color process. Dyeing of 100% cotton knit fabric with turquoise color using reactive dyes is a specialized and somewhat critical process due to the unique properties of turquoise dyes. Besides, required careful planning, as cotton is highly absorbent and knit structures are prone to creasing and uneven dyeing.

According to practical experience, I will discuss step by step 100% cotton knit fabric dyeing with turquoise color.

Process Flow Chart of 100% Cotton Knit Fabric Dyeing with Turquoise Color

Fabric loaded

Treating with anti-creasing agent (Room temperature)

Adding detergent

Adding antifoaming agent

Caustic dosing (dosing 6min)

Peroxide dosing (60˚c; 5min)

Run time 1 hour 95˚c

Sample check

If OK

Drain out

Normal hot (70˚c, 10min)

Drain

Adding Peroxide Killer

Run time 55˚c, 10min

Adding Acetic Acid

Run time 10min 55˚c (pH-4.5)

Adding enzyme

Run time 1hour, 55˚c

Enzyme hot- 70˚c, 10min

Drain

Filling in the tank (run time 5min)

Rinsing -4min

Drain

Filling in the tank

Adding Leveling, Antifoaming and Anti-creasing agent (R.T.)

10min run time (R.T.)

10min run time (60˚c)

Color dosing 30 min

10min run

½ Salt dosing-5min

½ Salt dosing 5 min

Runtime 25 min (60˚c)

Sample check

Soda dosing (2 g/l; 20min)

Remaining Soda dosing (30 min)

20 min run

Temp rise 80˚c

Run time 1 hour

Rinsing 5 min

Drain

Filling in the tank

Run time (RT)

Drain

Filling in the tank

Normal hot (60˚c, 10min)

Sample check

Drain

Adding Acetic Acid (room temp, run time 30 min)

Sample check

Drain

Filling in the tank

Adding soaping agent (90˚c, run 10 min)

Drain

Sample check

Filling in the tank

Rinsing (5 min room temp.)

Drain

Filling in the tank

Run time (5 min, room temp.)

Drain

Filling in the tank

Dosing-fixing agent (15 min)

Run time (20 min, room temp.)

Sample check

Drain

Filling in the tank

Dosing softener (5 min)

Run time (20 min, room temp.)

Sample check

Unload

Conclusion

Dyeing of 100% cotton knit fabric with turquoise color is a multi-stage process that requires precision and control. Each stage ensures uniform color, improved fabric softness, and lasting color fastness. Careful chemical dosing, temperature control, and sample checks guarantee a high-quality, vibrant, and durable finished fabric.